is not attained, but there is no difficulty in approaching it closely
enough to prevent the charge at any time rising above the level it
reached at first in the crucible, and this should be accomplished. It is
usual with quartzose ores to rely mainly on the action of carbonate of
soda, but not entirely. Litharge is also used; it forms, on fusion with
quartz, a silicate of lead, which is a yellow glass, easily fusible, and
more fluid in the furnace than silicate of soda is. By theory, 50 grams
of quartz would require 186 grams of litharge.[21] The reaction takes
place without evolution of gas, and in its working the only point is to
so regulate the heat that the litharge shall not fuse and drain under
the unattacked quartz, leaving it as a pasty mass on the surface. Now,
if in making up a charge for 50 grams of ore, we took 100 grams of
bicarbonate of soda (equivalent to about 63 grams of the carbonate),
this being five-sevenths of 140 grams (which by itself would be
sufficient), leaves two-sevenths of the quartz to be fluxed by other
reagents: two-sevenths of 186 grams (say 52 grams) of litharge would
serve for this purpose. But if we used 10 grams of borax, which has a
fluxing action about equal to that of the litharge, then 40 grams of the
latter, or (making an allowance for the quartz being not quite pure) say
35 grams, will suffice. The fluxes, then, for the 50 grams of ore would
be: bicarbonate of soda 100 grams, litharge 35 grams, and borax 10
grams; we could decrease any of these, and proportionately increase
either or both of the others, and still rely on getting a fusible slag,
which is the whole of the function of a flux, considered simply as a
flux. It should be remembered, however, that the slag is a bi-silicate
or acid slag, and that its acid character is increased by increasing the
proportion of borax.
But in addition to the fluxes there is required about 30 or 40 grams of
lead to collect the silver and gold. This is best added as litharge (say
40 grams) and flour (4 grams), or charcoal powder (2 grams). See pages
93 and 94. The full charge, then, would be:
Ore 50 grams.
Bicarbonate of soda 100 "
Litharge 75 "
Borax 10 "
Flour 4 "
Public-domain text, read in full here on John Shaqi.
Reviews
Reviews
No reviews yet
Be the first to share your thoughts on this work.
Elsewhere in the archive
Join the Discussion
Join the discussion
Sign in to leave a comment or review.
Sign InorCreate an account