Whilst, for the same material, from
which most of the gold has been extracted by "chloridising," 2.5 tons
each of ore, borax, and soda, 4 of litharge, and 4 grams of charcoal are
needed. This quantity requires a large crucible (I Battersea, round). In
this the proportion of silicate of soda and borax counted together is to
the oxide of iron as 4 to 1, on the supposition that the quartz and
oxide of iron of the ore are in about equal quantities; but, in the
larger charge especially, much oxide of lead would also remain as a
flux.
~Ores containing Sulphides.~--In assaying ores containing a large
proportion of pyrites or mispickel, or both, the best plan is to take a
portion and calcine so as to convert it into a product of the kind just
considered. The weighed portion of ore should be placed in a clean
crucible and be heated to incipient redness: with pyrites the first
effect is to drive off about half the sulphur as vapour which burns as
flame over the ore. At this stage care should be taken that there is no
great increase of temperature, otherwise there may be more or less
fusion, which would spoil the operation. When the sulphur flame ceases
the solid sulphide of iron burns with visible incandescence and the
charge should now be stirred with a flattened iron rod so as to expose
fresh portions to the air. The top of the furnace must be open, so that
air may have free access to the crucible. When stirring is no longer
followed by visible burning the heat may be raised to full redness. The
crucible is then lifted out (the stirrer still resting in it) and if the
charge gives off no odour of burning sulphur it is shaken out into an
iron mortar and mixed with the fluxes, taking care to clean the stirrer
in the mixture. The charge is then replaced in the crucible in which the
roasting was done and fused in the furnace. The resulting button of lead
is cupelled for fine metal. Ores rich in sulphides requiring this
treatment are frequently "concentrates." For their assay take 1 assay
ton (30 grams), calcine and mix with an equal weight of soda and of
borax (30 grams each), and half as much again of litharge (1.5 tons or
45 grams), and with 2 grams of charcoal or 5 grams of flour.
Public-domain text, read in full here on John Shaqi.
Reviews
Reviews
No reviews yet
Be the first to share your thoughts on this work.
Elsewhere in the archive
Join the Discussion
Join the discussion
Sign in to leave a comment or review.
Sign InorCreate an account