If you are treating the plate with nitrate of silver prepared as already
mentioned, clean the plate with dilute nitric acid, rub the surface with
the ball of amalgam, following with the swab and fairly rubbing in. It
will be well to prepare the plate some days before requiring to use it,
as a better adhesion of the silver and copper takes place than if
mercury is applied at once.
To amalgamate with zinc amalgam, clean the copper plate by means of a
swab, with fairly strong sulphuric acid diluted with water; then while
wet apply the zinco-mercury amalgam and well rub in. To prepare the zinc
amalgam, clip some zinc (the lining of packing cases will do) into small
pieces and immerse them in mercury after washing them with a little weak
sulphuric acid and water to remove any coating of oxide. When the
mercury will absorb no more zinc, squeeze through chamois leather or
calico (as for silver amalgam), and well rub in. The plate thus prepared
should stand for a few days, dry, before using. If, before amalgamation
with gold takes place, oxide of copper or other scum should rise on this
plate a little very dilute sulphuric acid will instantly remove it.
Sodium and cyanide of potassium are frequently used in dressing-plates,
but the former should be very sparingly employed, as it will often do
more harm than good by taking up all sorts of base metals with the
amalgam, and so presenting a surface which the gold will pass over
without adhering to. Where water is scarce, and is consequently used
over and over again, lime may be added to the pulp, or, if lime is not
procurable, wood ashes may be used. The effect is two-fold; the lime not
only tends to “sweeten” sulphide ores and keep the tables clean, but
also causes the water to cleanse itself more quickly of the slimes,
which will be more rapidly precipitated. When zinc amalgam is used,
alkalies would, of course, be detrimental.
Public-domain text, read in full here on John Shaqi.
Reviews
Reviews
No reviews yet
Be the first to share your thoughts on this work.
Elsewhere in the archive
Join the Discussion
Join the discussion
Sign in to leave a comment or review.
Sign InorCreate an account