Getting Gold: A Practical Treatise for Prospectors, Miners and StudentsJohnson, J. C. F. (Joseph Colin Francis)
History
Getting Gold: A Practical Treatise for Prospectors, Miners and Students
Johnson, J. C. F. (Joseph Colin Francis)
Gold mines and mining
About an ounce of silver to the foot of copper is sufficient. To apply
it on new plates use nitric acid applied with a swab to free the surface
of the copper from oxides or impurities, then rub the ball of amalgam
over the surface using some little force. It is always well when coating
copper plates with silver or zinc by means of mercury to let them stand
dry for a day or two before using, as the mercury oxidises and the
coating metal more closely adheres.
Only the very best copper plate procurable should be used for battery
tables; bad copper will always give trouble, both in the first "curing,"
and after treatment. It should not be heavily rolled copper, as the
more porous the metal the more easily will the mercury penetrate and
amalgamate. I cannot agree that any good is attained by scouring the
plates with sand and alkalies, as recommended in some books on the
subject; on the contrary, I prefer the opposite mode of treatment, and
either face the plates with nitrate of silver and nitrate of mercury,
or else with sulphate of zinc and mercury, in the form of what is
called zinc amalgam. If mine water, which often contains a little free
sulphuric acid, is being used, the latter plan is preferable.
The copper should be placed smoothly on the wooden table and secured
firmly thereto by copper tacks. If the plate should be bent or buckled,
it may be flattened by beating it with a heavy hammer, taking care to
interpose a piece of inch-thick soft wood between hammer and plate.
To coat with mercury only, procure some nitrate of mercury. This is
easily made by placing mercury in an earthenware bowl, pouring somewhat
dilute nitric acid on it, and letting it stand till the metallic mercury
is changed to a white crystal. Dense reddish-brown fumes will arise,
which are injurious if breathed, so the operation should be conducted
either in the open air, or where there is a draught.
Having your silvering solution ready, which is to be somewhat diluted
with water, next take two swabs, with handles about 12 inches long, dip
the first into a basin containing dilute nitric acid, and rub it rapidly
over about a foot of the surface of the plate; the oxide of copper will
be absolutely removed, and the surface of the copper rendered pure and
bright; then take the other swab, wet with the dilute nitric of mercury,
and pass it over the clean surface, rubbing it well in. Continue this
till the whole plate has a coating of mercury. It may be well to go
over it more than once. Now turn on the water and wash the plate clean,
sprinkle with metallic mercury, rubbing it upwards until the plate will
hold no more.
A basin with nitrate of mercury may be kept handy, and the plates
touched up from time to time for a few days until they get amalgamated
with gold, after which, unless you have much base metal to contend with,
they will give no further trouble.
Public-domain text, read in full here on John Shaqi.
Reviews
Reviews
No reviews yet
Be the first to share your thoughts on this work.
Elsewhere in the archive
Join the Discussion
Join the discussion
Sign in to leave a comment or review.
Sign InorCreate an account