The coarser grades of emery may be obtained by washing ordinary flour
of emery, but the finer ones have to be got from emery which has been
used in the previous processes. It is not a good plan to wash the
finer grades of emery out of the proceeds of very rough grinding say
with anything coarser than flour of emery--as there is a danger of
thereby contaminating the finer grades with comparatively coarse glass
particles (owing to their lightness) and this may lead to scratching.
If the finer grades are very light in colour, it may be inferred that
a considerable portion of the dust is composed of glass, and this does
no good. Consequently time may be saved by stirring up the
light-coloured mass with a little hydrofluoric acid in a platinum
capsule; this dissolves the finely divided glass almost
instantaneously. The emery and excess of hydrofluoric acid may then
be thrown into a large beaker of clean water and washed several times.
Fine emery thus treated has much the same dark chocolate colour as the
coarser varieties.
The operator should not wear a coat, and should have his arms bare
while working with fine emery, for a workshop coat is sure to have
gathered a good deal of dust, and increases the chances of coarse
particles getting between the surfaces.
Sec. 61. Details of the Process of Fine Grinding.
A lens of the size selected for description is mounted as before
mentioned on a leaden pedestal, and the operator places the latter on
a table of convenient height in a room as free from dust as possible.
Everything should be as clean as a pin, and no splashes of emery mud
should be allowed to lie about. I have found it convenient to spread
clean newspapers on the table and floor, and to wear clean linen
clothes, which do not pick up dust. I have an idea that in large
workshops some simpler means of avoiding scratches must have been
discovered, but I can only give the results of my own experience. I
never successfully avoided scratches till I adopted the precautions
mentioned.
Fig. 52.
The left hand should be employed in rotating the pedestal either
continuously (though slowly) or at intervals of, say, one minute.
This point is rather important. Some operators require two hands to
work the grinding tool, and in any case this is the safer practice.
Under these circumstances the pedestal may be rotated through
one-eighth or tenth of a revolution every three minutes, or
thereabouts. The general motion given to the grinding tool should be
a series of circular sweeps of about one-fourth the diameter of the
glass disc, and gradually carried round an imaginary circle drawn on
the surface of the lens and concentric with it (Fig. 52).
Public-domain text, read in full here on John Shaqi.
Reviews
Reviews
No reviews yet
Be the first to share your thoughts on this work.
Elsewhere in the archive
Join the Discussion
Join the discussion
Sign in to leave a comment or review.
Sign InorCreate an account