Nitrate of lead offers no advantages over the acetate, and is generally
more expensive to use. Free nitric acid is more objectionable than
free acetic acid, because it may act as a solvent on chrome yellow
and liberate free chromic acid, which is liable to “turn” the yellow.
When using lead nitrate it is preferable to neutralise potassium
bichromate with soda, to avoid the presence of free nitric acid. The
yellows mostly in demand are the inferior qualities, prepared by mixing
pure chrome yellows with white mineral matters, generally barytes,
gypsum, and kaolin, usually stirred in with the bichromate solution
before adding the lead salt. Barytes injures the colour least, but
kaolin has the advantage that it does not increase the weight of the
colour so much. Gypsum occupies an intermediate position; it is much
more voluminous than barytes, and does not injure the colour so much
as kaolin, but it is generally used together with barytes. It is not
advisable to use this combination, for the reason that the colour on
drying forms very hard pieces, which offer difficulties in grinding.
Gypsum, too, from being more easily acted on by reagents than barytes
or kaolin, tends to take part in the reaction by decomposing the
potassium bichromate before the addition of the lead salt, and this is
objectionable. (Weber.)
A writer in the _Chemical Trade Journal_ gives the following formula
for the production of various yellows:--
(1) For soluble lead salts:--
Kilos.
Lead acetate 100
Potassium bichromate 18
Sulphuric acid (66° B.) 12
This mixture yields a yellow of the formula PbCrO_{4}, PbSO_{4}. To
obtain good shades, the amount of water employed should not be less
than 1000 litres, or double as much with the nitrate. In the latter
case, it is better to neutralise the lead nitrate and to replace the
acid by the sulphate of an alkali or of magnesium, or preferably of
aluminium; for the neutralisation of the bichromate, the best substance
is magnesite. The formula thus becomes--Lead acetate and bichromate as
before; magnesite, 6 kilos.; aluminium sulphate, 27 kilos.
(2) The Basic Acetate Method.--Litharge, 76 kilos.; acetic acid (30 per
cent.), 42; bichromate, 21·5; sulphuric acid, 21·5; water, 2000 to 3000
litres. To obtain a denser chrome, 10 kilos. of soda should be added to
the acetate, and 5 of the sulphuric acid replaced by 10 of aluminium
sulphate. For the production of an orange chrome, the following
formula is given: Litharge, 76 kilos.; acetic acid (30 per cent.), 42;
bichromate, 24; Solvay’s soda, 15; and caustic soda (100 per cent.), 5.
Care must be taken that the temperature does not rise sufficiently high
to spoil the shade.
Public-domain text, read in full here on John Shaqi.
Reviews
Reviews
No reviews yet
Be the first to share your thoughts on this work.
Elsewhere in the archive
Join the Discussion
Join the discussion
Sign in to leave a comment or review.
Sign InorCreate an account