_Black._--Prepare the dye-bath with 3 lb. Triamine black B, 15 lb.
Glauber's salt, in fifty gallons of water. Dye exactly as in the
preceding recipe. Wash and rinse very thoroughly after lifting, then
diazotise in a bath of about 250 gallons of cold water, to which add
separately 2-1/2 lb. sodium nitrite dissolved in five times its bulk of
water and 8 lb. hydrochloric acid diluted. Enter the damp cotton and
treat it for about half an hour. Lift, pass through a weak acid bath,
rinse, and develop immediately in a bath of about 250 gallons of cold
water, containing 1 lb. developer T, 1 lb. soda, previously dissolved
together in hot water. Enter the damp goods, work well for half an hour,
then lift, wash and dry.
_Blue Black._--Dye with 4 lb. Diamine black B H, 2 lb. soda and 10 lb.
Glauber's salt, then diazotise and develop with naphthylamine ether.
_Dark Navy._--Dye with 3 lb. Diamine azo blue R R, 2 lb. soda and 10 lb.
Glauber's salt, then diazotise and develop with beta-naphthol.
_Light Chestnut Brown._--Dye with 2 lb. Cotton brown N, 1 lb. diamine
fast yellow A, 1 lb. soda and 10 lb. salt, then diazotise and develop
with phenylene diamine.
_Dark Brown._--Dye with 5 lb. Diamine cutch, 3 lb. soda and 20 lb.
Glauber's salt, then diazotise and develop with fast blue developer A D.
_Black._--Dye with 4 lb. Diamine black B H, 3 lb. soda and 20 lb.
Glauber's salt, diazotise and develop with 2 lb. resorcine and 1 lb.
phenylene diamine.
_Blue Black._--Dye with 4 lb. Diaminogene B, 2 lb. soda and 20 lb.
Glauber's salt, then diazotise and develop with beta-naphthol.
_Black._--Dye with 4-1/2 lb. Diaminogene B, 1/2 oz. Diamine fast yellow
B, 3 lb. soda and 20 lb. Glauber's salt, then diazotise and develop with
3 lb. resorcine and 1 lb. phenylene diamine.
_Light Blue._--Dye with 1-1/2 lb. Diaminogene blue B B, 1 lb. soda and
10 lb. Glauber's salt, then diazotised and develop with beta-naphthol.
_Maroon._--Dye with 6 lb. Primuline and 20 lb. salt, diazotise and
develop with blue developer A N.
_Olive Brown._--Dye with 5-1/2 lb. Diamine cutch, 3 lb. soda and 10 lb.
Glauber's salt, then diazotise and develop with fast blue developer A D.
_Gold Brown._--Dye with 1 lb. Cotton brown N, 3/4 lb. Diamine bronze G,
2 lb. soda and 10 lb. Glauber's salt, then diazotise and develop with
phenylene diamine.
_Walnut Brown._--Dye with 3 lb. Diamine brown M, 3 lb. soda and 20 lb.
Glauber's salt, then diazotise and develop with beta-naphthol.
_Brown._--Dye with 1-1/2 lb. Diamine brown M, 1 lb. Diamine fast yellow
B, 1 lb. cotton brown N, 1 lb. soda and 10 lb. Glauber's salt, then
diazotise and develop with phenylene diamine.
_Dark Plum._--Dye with 3 lb. Diamine brown V, 1 lb. soda and 10 lb.
Glauber's salt, then diazotise and develop with beta-naphthol.
_Black Brown._--Dye with 3 lb. Diamine cutch, 3 lb. Diamine black B H, 8
lb. soda and 20 lb. Glauber's salt, then diazotised and develop with
phenylene diamine.
Public-domain text, read in full here on John Shaqi.
Reviews
Reviews
No reviews yet
Be the first to share your thoughts on this work.
Elsewhere in the archive
Join the Discussion
Join the discussion
Sign in to leave a comment or review.
Sign InorCreate an account