_Measuring the deflection_: The method of measuring the
deflection should be such that any compression at the points of
support or at the application of the load will not affect the
reading. This may be accomplished by driving a small nail near
each end of the beam, the exact location being on the neutral
plane and vertically above each knife-edge support. Between
these nails a fine wire is stretched free of the beam and kept
taut by means of a rubber band or coiled spring on one end.
Behind the wire at a point on the beam midway between the
supports a steel scale graduated to hundredths of an inch is
fastened vertically by means of thumb-tacks or small screws
passing through holes in it. Attachment should be made on the
neutral plane.
The first reading is made when the scale beam is balanced at
zero load, and afterward at regular increments of the load which
is applied continuously and at a uniform speed. (See SPEED OF
TESTING MACHINE, above.) If desired, however, the load may be
read at regular increments of deflection. The deflection
readings should be to the nearest 0.01 inch. To avoid error due
to parallax, the readings may be taken by means of a reading
telescope about ten feet distant and approximately on a level
with the wire. A mirror fastened to the scale will increase the
accuracy of the readings if the telescope is not used. As in all
tests on timber, the strain must be continuous to rupture, not
intermittent, and readings must be taken "on the fly." The
weighing beam is kept balanced after the yield point is reached
and the maximum load, and at least one point beyond it, noted.
_Log of the test_: The proper log sheet for this test consists
of a piece of cross-section paper with space at the margin for
notes. (See Fig. 32.) The load in some convenient unit (1,000 to
10,000 pounds, depending upon the dimensions of the specimen) is
entered on the ordinates, the deflection in tenths of an inch on
the abscissæ. The increments of load should be chosen so as to
furnish about ten points on the stress-strain diagram below the
elastic limit.
As the readings of the wire on the scale are made they are
entered directly in their proper place on the cross-section
paper. In many cases a test should be continued until complete
failure results. The points where the various failures occur are
indicated on the stress-strain diagram. A brief description of
the failure is made on the margin of the log sheet, and the form
traced on the sketches.
_Disposal of the specimen_: Two one-inch sections are cut from
the region of failure to be used in determining the moisture
content. (See MOISTURE DETERMINATION, above.) A two-inch section
may be cut for subsequent reference and identification, and
possible microscopic study. The remainder of the beam may be cut
into small beams and compression pieces.
Public-domain text, read in full here on John Shaqi.
Reviews
Reviews
No reviews yet
Be the first to share your thoughts on this work.
Elsewhere in the archive
Join the Discussion
Join the discussion
Sign in to leave a comment or review.
Sign InorCreate an account