The method which is now used is to hang the hides in a closed chamber,
generally called a “sweat-pit,” Fig. 25, but usually constructed above
the ground-level and protected from sudden changes of temperature by
double walls, or by mounds of earth. The hides are hung in the
sweat-pit, in small chambers each capable of holding 50 or 100 hides.
The temperature is kept at about 15° to 20° C., the air being warmed, if
necessary, by the admission of steam below a perforated floor, or cooled
by a shower of water from sprinklers, so arranged as not to play
directly on the skins, and is thus always kept saturated with moisture.
Little if any ventilation is allowed, and a large quantity of ammonia is
given off from the decomposition of the organic matter, and no doubt
contributes to the solution of the epidermis and the loosening of the
hair, as the writer has found that ammoniacal vapours alone very
speedily produce this effect.
After 4-6 days of this treatment, the hair is sufficiently loosened to
be removed by working the skin over the beam with a blunt knife, or by
means of the stocks or hide-mill (see p. 116). Great care and
watchfulness are required to avoid injury to the grain by putrefaction.
The hide is in a slimy and completely flaccid and “fallen” condition,
and some trouble is occasioned by the hair being worked into the flesh
by the hide-mill, to obviate which, a slight liming is frequently given
after the sweating. Hides which have been unhaired in this way require
to be swollen by acid in the liquors in order to produce a satisfactory
sole-leather, as the sweating process does not swell or split up the
fibres.
In some European tanneries a similar process, but at a higher
temperature, is employed, and it is also largely used for sheep-skins
under the name of “staling,” but in this case is sometimes conducted in
a very rude and primitive manner, and frequently with the result of
considerable injury to the pelt.
The great objection to the sweating process, however carefully
conducted, is the liability of putrefaction to attack the skin itself,
causing “weak grain.” Its most advantageous use is for sole leather, as,
although the solution of the hide-substance may not be very much less
than in the case of liming, the dissolved matter remains in the hide
instead of being washed out, and being fixed by the tannin, contributes
to the solidity of the leather.
Public-domain text, read in full here on John Shaqi.
Reviews
Reviews
No reviews yet
Be the first to share your thoughts on this work.
Elsewhere in the archive
Join the Discussion
Join the discussion
Sign in to leave a comment or review.
Sign InorCreate an account