Either the one bath or two bath tannage (described on p. 108) may be
used, but, on the whole, the one bath method is preferred for the
following reasons: (1) Its application is easier; (2) it produces
a firmer and less elastic leather; and (3) there is practically no
danger of weakening the hide fibres. On the other hand, the two-bath
process produces a plumper leather which can, naturally, carry more
dressing and command a correspondingly better price. In skilled
hands, it is also under better control than the one-bath process,
while it is absolutely necessary for the popular pale bluish-grey
tint of chrome leather tennis soles.
[Illustration: FIG. 31
SUTCLIFFE SYSTEM OF DRYING]
The natural chrome sole requires very little dressing. The chromed
hides (usually rounded into butts or bends, shoulders and bellies)
are allowed to remain on a horse two or three days after the
completion of the tannage, so that the oxide of chromium may combine
more firmly with the fibres. They are then placed in the drum
tumbler again and washed in cold water for several hours. A constant
stream is conveyed to the drum through a rubber pipe fixed to the
tap, and escapes through small holes in the drum. The acid salts
are not thoroughly removed by this washing and must, therefore,
be neutralised with an alkali. Borax is the best for the purpose,
owing to its mild action on leather and antiseptic properties. From
1 to 2 per cent. borax on the weight of the leather is generally
sufficient, while, if soda be used for economical reasons, only
half the quantity is required. The drum is revolved for about an
hour; the liquor is then run off, and the leather receives a further
washing in cold water for half an hour, when it is in a condition to
receive the dressing, which is chiefly composed of materials which
help to fill and lubricate the interstices of the fibres so that
the substance is maintained and the natural strength of the fibres
preserved. Gelatine, pure glue, Tragasol, paraffin wax, carnauba wax,
spermaceti, Marseilles soap, are among the various ingredients used;
while the delicacy of the tint may be improved with china clay or
French chalk. Recipes vary considerably, each manufacturer claiming
to have secret methods. Solutions are made of the ingredients, or,
where one or more of the materials are insoluble, they are atomised
in a mixing pan before use. To induce thorough penetration, the
dressing liquid may be applied to the leather at a fairly high
temperature, as chrome leather is unaffected by heat which would
destroy the fibres of ordinary vegetable-tanned leather. Even so, it
is inadvisable to use a higher temperature than 170° F. The leather
is thoroughly impregnated with the dressing in about an hour's time,
and is then piled on a wooden horse for several hours, or overnight,
to drain and permit thorough incorporation of the dressing with the
leather. When well-drained, the grain of the hides is smoothed by
pressure with a special tool (Fig.
Public-domain text, read in full here on John Shaqi.
Reviews
Reviews
No reviews yet
Be the first to share your thoughts on this work.
Elsewhere in the archive
Join the Discussion
Join the discussion
Sign in to leave a comment or review.
Sign InorCreate an account