Within the vat, and working on the top of the copper plates, there is a
heavy copper stirrer or muller, B, Figs. 1 and 2, caused to revolve by the
shafting, C, at the rate of 45 revolutions per minute. At Huanchaca this
stirrer has been made with four projecting radial arms, D D, Figs. 1 and
2; but at Guadalupe it is composed of one single bell-shaped piece, Figs.
3 and 4, without any arms, but with slabs like arms fixed on its
underside; and this latter is claimed to be the most effective. The
stirrer can be lifted or depressed in the vat at will by means of a worm
and screw at the top of the driving shaft, Fig. 3.
The bevel gearing is revolved by shafting connected with pulley wheels and
belting, the wheels being 3 ft. and 1½ ft. in diameter, and 6 in. broad.
The driving engine is placed at one end of the building. Each vat requires
from 2½ to 3 horse-power, or in other words, an expenditure of 1
horse-power per ton of ore treated.
At the bottom of the vat, and in front of it, a large wooden stop-cock is
fitted, through which the liquid amalgam is drawn off at the end of the
process into another shallow-bottomed and smaller vat, Figs. 1 and 2.
Directly above this last vat there is a water hose, supplied with a
flexible spout, through which a strong stream of water is directed upon
the amalgam as it issues from the grinding vat, in order to wash off all
impurities.
The following is the mode of working usually employed. The grinding vat or
tina is first charged to about one-fifth of its depth with water and from
6 cwt. to 7 cwt. of common salt. The amount of salt required in the
process depends naturally on the character of the ore to be treated, as
ascertained by actual experiment, and averages from 150 lb. to 300 lb. per
ton of ore. Into this brine a jet of steam is then directed, and the
stirrer is set to work for about half an hour, until the liquid is in a
thoroughly boiling condition, in which state it must be kept until the end
of the process.
As soon as the liquid reaches boiling point, the stamped and roasted ore
is run into the vat, and at the end of another half-hour about 1 cwt. of
mercury is added, further quantities being added as required at different
stages of the process. The stirring is kept up continuously for eight to
twelve hours, according to the character and richness of the ores. At the
end of this time the amalgam is run out through the stop-cock at bottom of
the vat, is washed, and is put into hydraulic presses, by means of which
the mercury is squeezed out, leaving behind a thick, pulpy mass, composed
mainly of silver, and locally termed a "piña," from its resembling in
shape the cone of a pine tree. These piñas are then carefully weighed and
put into a subliming furnace, Figs. 5 and 6, in order to drive off the
rest of the mercury, the silver being subsequently run into bars. About
four ounces of mercury are lost for every pound of silver made.
Public-domain text, read in full here on John Shaqi.
Reviews
Reviews
No reviews yet
Be the first to share your thoughts on this work.
Join the Discussion
Join the discussion
Sign in to leave a comment or review.
Sign InorCreate an account