[7] From the molecular weights it will be seen that 74 grm. of
calcium hydrate, equivalent to 56 grm. of lime (CaO), require 73 grm.
of HCl gas for neutralization. This quantity of gas is contained
in 265 grm. of commercial hydrochloric acid of 18° Bé., or about
230 c.c.--that is, for 100 grm. CaO, 410 c.c. of 18° Bé. acid are
required; hence for the 100 kilos wet grain containing 400 grm. CaO,
1640 c.c. of acid are required for _complete neutralization_. It is
impracticable to use this amount of acid, for the reasons stated
above.
It will be noted that the quantity of acid used is only about one-tenth
of that required to neutralize completely the lime in the skin. If a
greater amount of acid be used the skins begin to absorb acid before
the lime in the interior is neutralized; but, provided the lime on the
surface of the skins is removed, that remaining in the interior is
forced out during the course of the bating process (see Chapter III.).
If more acid were used, then it would require to be added so slowly
that time would be wasted unnecessarily in doing the work.
With regard to the use of other acids for deliming, Lamb considers
formic acid preferable to hydrochloric, and states that the removal
of lime is more effectively accomplished by its use. He attributes
a pulling down action to the calcium formate produced, so that less
formic acid is required than would be equivalent to hydrochloric,
merely regarded as a solvent for lime. We shall refer to this point
again in Chapter II. It may be stated here that the author has obtained
better results by the use of a mixture of formic and acetic acid, in
equal proportions, than from either acid alone, but that the cost of
working is considerably greater than with hydrochloric acid.
Lactic acid is in fairly common use as a deliming agent. In practice
1 per cent. lactic acid (50 per cent. strength) calculated on the wet
weight of pelt, is used, added gradually in small quantities. This does
not remove the whole of the lime, but sufficient for the skins to puer
quickly.
Some tanners measure their acid per dozen skins. In a case which came
under my notice, 1200 c.c. 90 per cent. formic acid were being used for
ten dozens medium goat skins at a temperature of 35° C., time 1-1/4
hours.
The following table, due to Professor H. R. Procter,[8] gives the
cost of dissolving 1 lb. of lime at present approximate prices of
the various acids. The dissociation constant K shows their relative
“strength;”[9] the equivalent, Eq., the weight in lb. of 100 per cent.
acid required to dissolve 28 lb. of lime. Ordinary wet limed hides,
unhaired and fleshed, contain only about 4 lb. lime per 1000 lb. wet
weight.
[8] Tanners’ Year Book, 1911, p. 59.
[9] See Chapter III.
COST OF ACIDS TO REMOVE 1 LB. LIME.
Public-domain text, read in full here on John Shaqi.
Reviews
Reviews
No reviews yet
Be the first to share your thoughts on this work.
Join the Discussion
Join the discussion
Sign in to leave a comment or review.
Sign InorCreate an account