Take a $2 50c. piece of gold, and put it into a mixture of 1 ounce
of nitric and 4 ounces of muriatic acids, (glass vessels only are to
be used in this work,) when it is all cut dissolve 1/2 an ounce of
sulphate of potash in one pint of pure rain water, and mix the gold
solution, stirring well; then let stand and the gold will be thrown
down; then pour off the acid fluid, and wash the gold in two or
three waters, or until no acid is tasted by touching the tongue to
the gold. Now dissolve one ounce of cyanuret of potassium in one
pint of pure rain water, to which add the gold, and it is ready to
use. Clear the article to be plated from all dirt and grease with
whiting and a good brush; if there are cracks it may be necessary
to put the article in a solution of caustic potash. At all events
every particle of dirt and grease must be removed; then suspend the
article in the cyanuret of gold solution, with a small strip of zinc
cut about the width of a common knitting needle, hooking the top
over a stick which will reach across the top of the vessel or bottle
holding the solution. If the zinc is too large the deposit will be
made so fast that it will scale off. The slower the plating goes on
the better, and this is arranged by the size if the zinc used. When
not using the plating fluid keep it well corked and it is always
ready to use, bearing in mind that it is poison as arsenic, and
must be put high out of the way of children, and labelled poison,
although you need have no fear using it; yet accidents might arise
if its nature were not known.
9. ELECTRO SILVERING--USUAL METHOD
This is done every way the same as gold plating (using coin) except
that rock salt is used instead of the cyanuret of potassium to
hold the silver in solution for use, and when it is of the proper
strength of salt it has a thick curdy appearance, or you can add
salt until the silver will deposit on the article to be plated,
which is all that is required. No hesitation need be felt in trying
these receipts, as they are obtained from a genuine source, and are
in every day use.
10. GOLD PLATING FLUID
Warm six ounces of pure rain water, and dissolve in it 2 ounces of
cyanide of potassium, then add a 1/4 ounce oxide of gold; the
solution will at first be yellowish, but will soon subside to white;
then half fill a bottle with whiting, fill it up with this solution
and shake it well; you may now take a piece of old cotton, wet it
with the solution, rub it well over brass, copper, &c., and it is
nicely washed with gold.
11. SILVER PLATING FLUID
Public-domain text, read in full here on John Shaqi.
Reviews
Reviews
No reviews yet
Be the first to share your thoughts on this work.
Join the Discussion
Join the discussion
Sign in to leave a comment or review.
Sign InorCreate an account