The Manufacture of Paper: With Illustrations, and a Bibliography of Works Relating to Cellulose and Paper-MakingSindall, R. W. (Robert Walter)
History
The Manufacture of Paper: With Illustrations, and a Bibliography of Works Relating to Cellulose and Paper-Making
Sindall, R. W. (Robert Walter)
Papermaking
This change is due to the gradual oxidation of the constituents of
the paper, the ligno-cellulose of the mechanical wood pulp being most
readily affected by the high temperature, and the pure cellulose of the
rag paper being least altered.
The process of oxidation, brought about rapidly under the conditions of
the experiment described, takes place in papers of low quality exposed
to air in the ordinary circumstances of daily use, but of course at an
extremely slow rate. The deterioration of such paper is not, however,
due to the simple oxidation of the cellulose compounds, because other
factors have to be taken into account. The presence of impurities in
the paper on the one hand, and of chemical vapours in the air on the
other, hastens the decay of papers very considerably.
_Percentage of Cellulose in Fibrous Plants._--The value of a vegetable
plant for paper-making is first determined by a close examination
of the physical structure of the cellulose isolated by the ordinary
methods of treatment. If the fibres are weak and short, the raw
material is of little value, and it is at once condemned without
further investigation, but should the fibre prove suitable, then the
question of the percentage of cellulose becomes important.
There are several methods employed for estimating the amount of
cellulose in plants. The process giving a maximum yield is known as the
chlorination method, the details of which are as follows:--About ten
grammes of the air-dried fibre is dried at 100° C. in a water oven for
the determination of moisture. A second ten grammes of the air-dried
fibre is boiled for thirty minutes with a weak solution of pure caustic
soda (ten grammes of caustic soda in 1,000 cubic centimetres of water),
small quantities of distilled water being added at frequent intervals
to replace water lost by evaporation. The residue is then poured on to
a piece of small wire gauze, washed thoroughly, and squeezed out. The
moist mass of fibre is loosened and teased out, placed in a beaker,
and submitted to the action of chlorine gas for an hour. The bright
yellow mass is then washed with water and immersed in a solution of
sodium sulphite (twenty grammes of sodium sulphite in 1,000 cc. of
water). The mixture is slowly heated, and finally boiled for eight to
ten minutes, with the addition of 10 cc. of caustic soda solution. The
residue is washed, immersed in dilute sodium hypochlorite solution
for ten minutes, again washed, first with water containing a little
sulphurous acid and then with pure distilled water. It is finally dried
and weighed.
Public-domain text, read in full here on John Shaqi.
Reviews
Reviews
No reviews yet
Be the first to share your thoughts on this work.
Join the Discussion
Join the discussion
Sign in to leave a comment or review.
Sign InorCreate an account